1. Where the ammonia comes from
In dairy sheds and feedlots, urease enzymes in manure hydrolyse the urea in cattle urine, releasing ammonia gas continuously. The ammonia dissolves into the moisture film on wire surfaces, creating a persistently alkaline, complexing environment (pH ≈ 9–11).
The root cause is protein. Animal feed protein is roughly 16% nitrogen by mass; that nitrogen is excreted as urea (mammals) or uric acid (poultry), which bacteria break down to ammonia. So the higher the protein intake and stocking density, the more ammonia is released — poultry and pigs are the most aggressive environments, followed by housed dairy cattle, with sheep on open pasture the mildest.
2. How zinc normally protects itself
In ordinary atmospheres, zinc corrodes slowly and its corrosion products build a dense protective patina — this is why galvanising works so well in standard rural conditions.
3. What ammonia does to that film
Ammonia is a strong ligand for zinc. It dissolves the protective layer by forming the soluble tetraammine-zinc complex — so the film is stripped as fast as it forms, fresh zinc is re-exposed, and corrosion becomes a continuous linear loss of metal.
This is why a heavier coating doesn't solve the problem. Specifying 240 g/m² of zinc instead of 150 g/m² just means more sacrificial metal to consume — the consumption rate stays the same. The issue is the mechanism, not the mass.
4. Why the Zn-Al coating resists
Pure zinc (HDG)
- Zn2+ forms soluble ammine complexes — the protective film is constantly dissolved
- Continuous, linear metal loss in NH3-laden atmospheres
- Heavier coating = longer countdown, same endpoint
Zn-10%Al (ZA)
- Al3+ forms no stable ammine complex — ammonia cannot dissolve the alumina (Al2O3) passive film
- Ammonia is a weak base (pH ≤ ~11) — far too weak to attack Al2O3, which requires pH > 13
- Corrosion products form dense Zn-Al layered double hydroxides (LDH) — the film becomes more stable over time
Coating composition can materially affect corrosion behaviour in ammonia-laden environments. Buyers should specify the required coating, test evidence and exposure assumptions rather than rely on a universal service-life multiple.
Specifying for high-ammonia country?
YieldMax fixed knot fence is available with Zn-Al (Type ZA) and hot-dip galvanised wire options. Confirm the required standard, coating class, coating mass and order-specific documentation before production.
This summary is provided by YieldMax for planning purposes. Coating types and classes referenced follow AS/NZS 4534; the published standard remains the authoritative reference.